CAUSE SOLUTION
Problem: Glossy Bond Line
Inadequate temperature Increase temperature
Lack of pressure Increase pressure
Problem: Chalking
Adhesive, stock or plant at low temperature ideal bonding at 65°f (18°c) temp.
Problem: Adhesive On Only One Surface (No Transfer)
Poor joint Improve joint
Long open time Lower open time
Precure Check moisture content or shorten assembly time
Low pressure Increase pressure to recommended
Problem: Dark Stain In Adhesive Joint
Iron contamination Check to see if adhesive is in contact with iron materials such as drums or equipment parts
Problem: Telegraphing To Face
Dirt, chips, etc. On core surface Keep laminating area clean
Surface defects on materials Clean and inspect surface before laminating
Differential density Press at minimum safe pressure and check thickness of lumber band relative to core
Improper spreader grooving Check recommended spread rate
Excessive pressure Reduce pressure
Poor veneer splice lines Be sure they have intimate contact